In this paper, a cylindrical 9Ah aluminum shell lifepo4 lithium iron phosphate graphite battery is used as the research object. The changes in battery capacity, voltage, and AC resistance during and after storage at 55/45/23 and -10 ° C are studied. The parameters of DC internal resistance, power capability, constant current charge ratio, coulomb / energy efficiency, etc. before and after storage at 45/23 ° C were tested, and the impact of these parameter changes on the performance of the battery pack was analyzed. The best storage method of lifepo4 lithium iron phosphate graphite system power battery is given.
The test is a cylindrical 32131 aluminum shell lifepo4 lithium iron phosphate graphite battery as the research object, with a rated capacity of 9Ah. The positive and negative active materials are lifepo4 lithium iron phosphate and artificial graphite, respectively. 45/55 ℃ storage use DHP200 type electric thermostatic incubator; low temperature use low temperature refrigerator; electrical performance test equipment is CT-3008W-5V100A-TF test cabinet; AC internal resistance test equipment is HIOKI3554 battery internal resistance tester, AC1kHz.
Battery storage experiment one
(1) Select ≥60 single-cell batteries, charge and discharge for 3 weeks at a temperature of 3.65 ~ 2V with a current of 4500mA (0.5C) at room temperature, and obtain the capacity value of the battery before the test. Finally, the battery capacity is 100%, 50%, The 0% SOC state (20 batteries per SOC) is completed to stabilize the capacity. After being left for 15 hours, measure the basic data such as voltage and AC internal resistance to be tested;
(2) Select 4 batteries with 100%, 50%, and 0% SOC status and place them in a 55 ° C oven for 28 days. Select 4 batteries with 100%, 50%, and 0% SOC status and leave 12 batteries. Place in a 45 ° C oven for 28 days; select 4 100%, 50%, and 0% SOC batteries in total and place 12 batteries in a 23 ° C air-conditioned house for 28 days; select 4 100%, 50%, and 0% respectively In the SOC state, a total of 12 batteries were stored in a -10 ° C refrigerator for 28 days. During the storage process, these batteries were tested for internal resistance and voltage every 7 days;
(3) After the battery is put aside, put the battery on the test cabinet and put the charging cycle in the range of 3.65 ~ 2V for 3 weeks with the current of 4500mA (0.5C) at room temperature to get the battery capacity after storage.
Data and discussion: Experiment 1, storage of battery voltage, internal resistance and capacity change during 28 days
Figure 1 shows the change in the voltage (open circuit voltage) of the experimental battery during storage for 28 days. From Figure 1, it can be seen that the open circuit voltage change during storage at different temperatures and different SOC states is not obvious. The best consistency is at 50 In the% SOC state, the biggest change is in the 0% SOC state. This has a lot to do with the polarization of lifepo4 lithium iron phosphate graphite system batteries in different SOC states. Generally, this series of batteries has the largest polarization at 0% SOC, and the least polarization at 50% SOC. It can also be seen from the voltage change relationship at different temperatures of 0% SOC in FIG. 1 that the temperature increase is beneficial to the battery to quickly reach a stable state after polarization. Using this principle, when the battery vehicle module is assembled, the batteries with similar polarization status can be quickly selected by heating up.
Figure 1 Variation of battery voltage (V) during 28 days of storage
The change of the AC internal resistance during the storage of the experimental battery for 28 days is shown in Figure 2. It can be seen from Figure 2 that the AC internal resistance test value decreases with increasing temperature. This is because the higher the temperature, the The stronger the electrical conductivity. However, after storage, return to normal temperature and test again. The internal resistance of all batteries is not much different, but the AC internal resistance of the battery changes after storage at different SOCs and temperatures are relatively obvious. The internal resistance of the battery after storage at a high temperature of 45/55 ° C and 100% SOC increased significantly. This is because after storage at high temperature and high SOC, the SEI on the graphite anode surface in the lifepo4 lithium iron phosphate / graphite system battery became thicker, and the electrolyte LiPF6 The slight decomposition causes the SEI components to form inorganic salts such as LiF with high resistance.
Figure 2 AC internal resistance (mΩ) of the battery during 28 days of storage
Table 1 lists the battery capacity change data after 28 days of storage. From the data, it can be seen that compared to the high SOC state, low SOC is more conducive to battery capacity storage. From the data, it can be seen that except for low temperature 0% SOC,- In addition to the loss of capacity at 10 ° C, the battery capacity in other 0% SOC states has increased to a certain extent. This phenomenon may be due to the secondary particles of the positive electrode material cracking after storage, forming a fresh interface. It has the activity of deintercalating lithium ions again. In fact, this phenomenon also occurs in batteries that are directly cycled without storage. The capacity of these batteries is gradually increasing during the initial dozens of weeks of cycling.
Table 1 Storage capacity data table before and after 28 days
Battery storage experiment two
(1) Select ≥45 single-cell batteries, charge and discharge at a temperature of 3.65 ~ 2V for 3 weeks at a temperature of 9000mA (1C) at room temperature, obtain the capacity value of the battery before the test, and follow the HPPC (5C) in the Freedom CAR standard. (Release 3.75C feedback) test method to test the battery, and finally ended with 100%, 80%, 50%, 30%, O% SOC state (9 batteries of each SOC), after leaving for 15 hours, measure its voltage, AC internal Resistance and other basic data to be tested;
(2) Select 3 batteries of 100%, 80%, 50%, 30%, and 0% SOC respectively, and place them in a 45 ° C oven for three months; select 3 batteries of 100%, 80%, and 50% respectively. A total of 15 batteries at 30%, 0% SOC status were placed in a 23 ° C air-conditioned house for three months; during the shelving process, these batteries were tested for AC internal resistance, 1 C capacity, and HPPC every 28 days.
Data and discussion: Change in AC internal resistance of the battery during the three months of experiment two
Figures 3 and 4 show the change curves of the internal resistance of AC batteries with different SOCs (100%, 80%, 50%, 30%, and 0%) during 25 months at 25 and 45 ° C. It can be seen from the two figures that the increase in AC internal resistance of the battery left at a high temperature of 45 ° C is significantly higher than that of a battery left at 25 ° C, which is consistent with the results of Experiment 1. In addition, we also found that the battery storage SOC that has the least impact on battery AC internal resistance is different at different temperatures. At 25 ° C, the minimum impact SOC is 80% SOC, and at 45 ° C, the AC internal resistance after storage of each SOC is different. The increase is large, the relatively small is 30% SOC. It was reported in [5] that the change in the internal resistance of the AC during battery shedding was mainly the change of the charge transfer resistance of the positive electrode LiFePO4 with temperature and SOC. From our test results, the positive electrode LiFePO4 charge transfer resistance increases with temperature, the faster the change in SOC from the middle (30% to 80% SOC) to both ends (0%, 100%). When the two factors work together on the battery, the results shown in Figures 3 and 4 are shown, and the SOC with less effect on the battery internal resistance at different temperatures is different.
Figure 3 AC internal resistance change rate of the battery during storage at 25 ℃ for three months
Figure 4 AC internal resistance change rate of the battery during storage at 45 ° C for three months
Data and discussion: Change of battery 1C capacity during 3 months of test 2 storage
Figure 5 and Figure 6 respectively show the 1C capacity change rate curves of different SOC (100%, 80%, 50%, 30%, 0%) batteries during three months of storage at 25 and 45 ° C. It can be seen that the battery 1C capacity decay after being left at a high temperature of 45 ° C is significantly higher than that of a battery left at 25 ° C, which is also consistent with the results of Experiment 1. Storage at 0% SOC has the least impact on battery capacity decay.
Figure 5 1C capacity change rate of the battery during three months of storage at 25 ° C
Figure 6 1C capacity change rate of the battery during three months of storage at 45 ° C
The change of LiFePO4 / graphite system power battery capacity during storage is mainly caused by the following three factors:
(1) The formation of the irreversible capacity of the negative electrode is mainly due to the increase in storage time. Part of the lithium embedded in the negative electrode graphite layer loses its activity and becomes dead lithium, which cannot be returned to the positive electrode through discharge. The impact is negative, so as SOC increases, more capacity will be lost for this reason;
(2) According to Ohm's law: U = UR + Ur = I (R + r), where: U is the battery electromotive force; UR is the circuit terminal voltage; Ur is the battery internal voltage; R is the external circuit resistance; r is the battery itself Internal resistance; I is the discharge current. Due to the influence of the increase in internal resistance during the shelving process; the increase, the terminal voltage decreases, the terminal voltage arrives early during discharge, and the discharge time decreases compared to the initial storage period, which reduces the discharge capacity. This effect is also negative;
(3) As the storage time of the positive electrode LiFePO4 increases, the secondary particles crack, forming a fresh interface and regaining the activity of deintercalating lithium ions. This effect is positive, so the increase in capacity may occur in the initial stage of storage. . From the above three points of analysis, it can be seen that the experimental data is the final result after integrating these three effects.
Data and discussion: The change of DC internal resistance of the battery during the three months of experiment two
Figures 7 and 8 show the DC internal resistance change curves of different SOC (100%, 80%, 50%, 30%, 0%) batteries during the three months of storage at 25 and 45 ° C. It can be seen from the two figures that the DC internal resistance of the battery left at a high temperature of 45 ° C is slightly lower than that of a battery left at 25 ° C. The change of DC internal resistance with SOC is similar at different temperatures. The increase rate is O%,
100%, 30%, 80% and 50% SOC.
Figure 7 DC internal resistance change rate of the battery during storage for three months at 25 ° C
Figure 8 DC internal resistance change rate of the battery during storage at 45 ° C for three months
Data and discussion: battery power capacity changes during the three months of experiment two
Figure 9 Change rate of battery discharge power capacity during three months of storage at 25 ° C
Figure 10 Change rate of battery discharge power capacity during storage at 45 ° C for three months
Figure 11 Change rate of battery feedback power capability during storage for three months at 25 ° C
Change rate of battery's feedback power capability during storage at 12 ° C for three months
Figure 9, Figure 10, and Figure 11 and Figure 12 show the discharge power of the batteries with different SOC (100%, 80%, 50%, 30%, 0%) during the three months of storage at 25 and 45 ° C, respectively. The capacity change rate and the feedback power capacity change rate curve. Comparing the two figures, it can be seen that the DC internal resistance of the battery left at a high temperature of 45 ° C is slightly lower than that of a battery left at 25 ° C. The change of power capacity with SOC is similar at different temperatures. The increase rates are 0%, 100%, 30%, 80%, and 50% SOC from high to low, respectively.
From the above results, the change of battery power capacity is exactly the same as the change of battery DC internal resistance. This is because the change of power battery power capacity depends on the change of battery DC internal resistance. The most direct reflection during charging and discharging. Battery DC internal resistance is mainly composed of ohmic internal resistance and activation impedance. The change law of ohmic internal resistance is numerically similar to the change of AC internal resistance. Therefore, both the change of DC internal resistance and the change of AC internal resistance follow the SOC. The 30% ~ 80% SOC in the middle part increases more rapidly with changes in both ends (0%, 100%), but the activation impedance is slightly more affected by the temperature. The higher the temperature, the smaller the activation energy, that is, the smaller the activation impedance. . Therefore, the test data reflects that the DC internal resistance of the battery left at 45 ° C is slightly lower than that of the battery left at 25 ° C.
result
By testing the battery performance changes such as AC internal resistance, capacity, DC internal resistance, and power capacity after the battery is left at different temperatures and different SOCs, it is found that the laws of various performance changes during battery storage are different. In actual storage, you need to choose the appropriate storage conditions according to the length of the storage time and the direction of use of the battery. For example, when the battery is used at a high frequency in terms of power capacity, in order to ensure the power capacity, it is necessary to appropriately increase the storage temperature, and when the battery is used only under a low rate simple charge and discharge condition, a lower storage temperature can be selected. Based on the above test results, the charge state of 50% SOC at room temperature is a storage state that is more conducive to the performance of the battery.